Influence of Poling Conditions on Properties of BaTiO3 Single Crystal

Abstract
A BaTiO3 single crystal, whose dimensions were 3.9×3.9×3.6 mm3, was mechanically and electrically poled to remove its 90° and 180° ferroelectric domain walls, respectively. After mechanical poling, four-step electrical poling was applied to the crystal, which did not include 90° domain walls, with the aim of removing the 180° domains gradually. In each of these steps, the dielectric constant of the crystal was measured using an impedance analyzer. Prior to the electrical poling, the dielectric constant in the [001] direction was 137 at 100 kHz (unclamped) and 133 at 10 MHz (clamped). By applying four-step poling, these values varied gradually with the progress of poling, and became 130 and 58, respectively, after the final step, i.e., in a single-domain state.

This publication has 2 references indexed in Scilit: